Min. Order: 10
40CrNiMoAalloy steelnickle steelalloy structural steel:40CrNiMoA
standard:GB/T 3077-1988
●Chemical composition:
碳 C :0.37~0.44
硅 Si:0.17~0.37
锰 Mn:0.50~0.80
硫 S :allow remains content≤0.025
磷 P :allow remains content≤0.025
铬 Cr:0.60~0.90
镍 Ni:1.25~1.65
铜 Cu:allow remains content≤0.025
钼 Mo:0.15~0.25
●mechanical properties:
tensile strength σb (MPa):≥980(100)
yield strength σs (MPa):≥835(85)
extensibility δ5 (%):≥12
reduction of area ψ (%):≥55
ballistic work Akv (J):≥78
notched bar impact strength αkv (J/cm2):≥98(10)
rigidity :≤269HB
specimen size:specimen size of rough 25mm
●heat treatment regime and metallurgical structure:
heat treatment regime :quenching 850℃,oil cooling ;backfire 600℃,water cooling 、oil cooling.
●deliver position :heat treatment(normalizing、annealing or high-temperature backfire)or no heat treatment, this should be shown on the contract.
website http://www.testeel.com